Printing here with eSun PLA at 215 C on a Prusa Mini, and there are lots of hairline strings.

What's causing those strings? Temp too low?

you are viewing a single comment's thread
view the rest of the comments
[-] rambos@lemm.ee 5 points 11 months ago

You already got a good answer about lowering temp and tuning retraction. Other than that, you have underextrusion there (gaps in the flat part on the build plate). I think you should extend your calibration:

Calibrate temp - flow - retraction

To reduce stringing you want:

  • lower temp
  • higher retraction
  • faster travel speed

Be careful with first two, if you go too far you might get a clog. Sometimes its just better to accept some stringing, but since you are at 215 I bet it can be improved quite easy

this post was submitted on 16 Nov 2023
49 points (98.0% liked)

3DPrinting

15493 readers
192 users here now

3DPrinting is a place where makers of all skill levels and walks of life can learn about and discuss 3D printing and development of 3D printed parts and devices.

The r/functionalprint community is now located at: !functionalprint@kbin.social or !functionalprint@fedia.io

There are CAD communities available at: !cad@lemmy.world or !freecad@lemmy.ml

Rules

If you need an easy way to host pictures, https://catbox.moe may be an option. Be ethical about what you post and donate if you are able or use this a lot. It is just an individual hosting content, not a company. The image embedding syntax for Lemmy is ![](URL)

Moderation policy: Light, mostly invisible

founded 1 year ago
MODERATORS